[ABSTRAK
Penelitian ini bertujuan untuk membandingkan kuat rekat geser dan Adhesive
Remnant Index (ARI) dua produk breket metal yang direkatkan dengan satu adesif.
Dua puluh gigi premolar atas manusia ditanam pada silinder PVC dengan resin
akrilik. Spesimen dibagi menjadi dua kelompok, kelompok A: breket metal 3B, Cina
+ Transbond XT; kelompok B: breket metal Protect, Cina + Transbond XT (3M,
Unitek, Amerika). Dihasilkan rerata kuat rekat geser 6,09 dan 7,91 MPa pada
kelompok A dan B (p<0,05) dan nilai ARI: 1 dan 2 pada kedua kelompok (p>0,05).
Disimpulkan bahwa dua kelompok memiliki nilai kuat rekat geser yang berbeda
bermakna dengan kegagalan ikatan bersifat kohesif
ABSTRACT
The aims of this study were to compare in vitro shear bond strength (SBS)
and Adhesive Remnant Index (ARI) of two metal bracket products bonded with an
adhesive material. Twenty human upper first premolar embedded in acrylic resin.
Specimens were divided into two groups, Group A: 3B, China metal bracket +
Transbond XT; Group B: Protect, China metal bracket + Transbond XT (3M,
Amerika). The mean SBS for Group A and B were 6,09 dan 7,91 MPa and ARI: 1
and 2 (p>0,05). It was concluded that the SBS of two groups was significantly
different with cohesive bond failure.;The aims of this study were to compare in vitro shear bond strength (SBS)
and Adhesive Remnant Index (ARI) of two metal bracket products bonded with an
adhesive material. Twenty human upper first premolar embedded in acrylic resin.
Specimens were divided into two groups, Group A: 3B, China metal bracket +
Transbond XT; Group B: Protect, China metal bracket + Transbond XT (3M,
Amerika). The mean SBS for Group A and B were 6,09 dan 7,91 MPa and ARI: 1
and 2 (p>0,05). It was concluded that the SBS of two groups was significantly
different with cohesive bond failure., The aims of this study were to compare in vitro shear bond strength (SBS)
and Adhesive Remnant Index (ARI) of two metal bracket products bonded with an
adhesive material. Twenty human upper first premolar embedded in acrylic resin.
Specimens were divided into two groups, Group A: 3B, China metal bracket +
Transbond XT; Group B: Protect, China metal bracket + Transbond XT (3M,
Amerika). The mean SBS for Group A and B were 6,09 dan 7,91 MPa and ARI: 1
and 2 (p>0,05). It was concluded that the SBS of two groups was significantly
different with cohesive bond failure.]

 File Digital: 1

Shelf
 S-Fanny Anduari Dianty.pdf :: Unduh

LOGIN required

 Metadata

Jenis Koleksi : UI - Skripsi Membership
No. Panggil : S-Pdf
Entri utama-Nama orang :
Entri tambahan-Nama orang :
Entri tambahan-Nama badan :
Program Studi :
Subjek :
Penerbitan : [Place of publication not identified]: Fakultas Kedokteran Gigi Universitas Indonesia, 2015
Bahasa : ind
Sumber Pengatalogan : LibUI ind rda
Tipe Konten : text
Tipe Media : computer
Tipe Carrier : online resource
Deskripsi Fisik : xiii, 62 pages : illustration ; 28 cm +Appendix
Naskah Ringkas :
Lembaga Pemilik : Universitas Indonesia
Lokasi : Perpustakaan UI, Lantai 3
  • Ketersediaan
  • Ulasan
  • Sampul
No. Panggil No. Barkod Ketersediaan
S-Pdf 14-17-625925108 TERSEDIA
Ulasan:
Tidak ada ulasan pada koleksi ini: 20421425
Cover